Background: Esthetic treatment is the options of patient seeking orthodontic treatment. Therefore this study was conducted to measure the concentration of Aluminum, Nickel, Chromium and Iron ions released from combination of monocrysralline brackets with different arch wires immersed in artificial saliva at different duration, to evaluate the corrosion point on different parts of the orthodontic appliances before and after immersion in artificial saliva, and to evaluate the corrosion potential of each group of the orthodontic appliances. Material and methods: Eighty orthodontic sets prepared. Each set represents half fixed orthodontic appliance, from the central incisor to the first molar, for the maxillary arch, each set consisted of molar band, five brackets, half arch wire and ligature elastic.These sets are divided into two groups: Group A: with monocrystalline brackets divided into five subgroups (each subgroup has ten sets), but differ in arch wires, as numbered stainless steel, nickel-titanium, thermally activated, coated stainless steel and coated nickel-titanium arch wires respectively. Group B: with stainless steel brackets divided into three subgroups (also each subgroup has ten sets), but differ in arch wires, as numberedstainless steel, nickel-titanium, and thermally activated arch wires respectively. Used optical microscope to check the corrosion points, and used potentiostat techniques to indicate corrosion rate and tendency. Results: The greatest concentration of Aluminum and nickel ions release during the 1st week in group A, then sharply decreased in the 2nd week. The release of chromium ion released increase with increase intervals, while iron ion released decrease with increase time. Both nickel and chromium ions increase with increase intervals in group B,while iron increase to the maximum at 3rd weeks, then began to degrease. Optical microscope displayed pitting, crevices, and intergranular corrosion. Potentiostat techniques indicated that increase corrosion when used stainless steel and coated nickel titanium than others arch wires with group A, while corrosion increase with nickel titanium than stainless steel arch wires with group B. Conclusions: Non-significant difference in the total nickel, chromium and iron release in group B. Aluminum and iron increase in A4 and A5, while nickel and chromium increase in A1 and A2.The total released amounts of metals ions in both groups were less than the amounts of daily intake.
The makers of strife exist in every era and time. They differ in how these temptations are created and the methods used in doing so. In our modern era, they are more; This is due to the presence of information technology and its easy availability at their fingertips, as well as the spread of social networking sites, which are rapidly spreading among ignorant groups and groups that are deficient in their use. Which led the makers of sedition to exploit these matters and create various temptations and spread them among peoples and societies. Today, we cannot predict the future of humanity in light of this huge amount of temptation. What the Holy Qur’an mentioned about the types of temptations in its noble verses and their embodiment in seve
... Show MoreMost of us are tired of the circumstances that surround us because of their deficiency, deprivation, and sullenness, even though troubles and pains are the soil in which the seeds of strong personality sprout.
The content of the research is summed up in the fact that there is no need to frown, so let our face be free, and our word good and tolerant, so that we can be the most loving people of those who give them, and the Messenger of God (may God’s prayers and peace be upon him and his family) was known to be the heaviest concerns of people, but he was most smiling of people, by smiling, we buy lives, so we should get used to it, because that gives us hope and finds the world in our hands, an
... Show MoreThe risk assessment for three pipelines belonging to the Basra Oil Company (X1, X2, X3), to develop an appropriate risk mitigation plan for each pipeline to address all high risks. Corrosion risks were assessed using a 5 * 5 matrix. Now, the risk assessment for X1 showed that the POF for internal corrosion is 5, which means that its risk is high due to salinity and the presence of CO, H2S and POF for external corrosion is 1 less than the corrosion, while for Flowline X2 the probability of internal corrosion is 4 and external is 4 because there is no Cathodic protection applied due to CO2, H2S and Flowline X3 have 8 leaks due to internal corrosion so the hazard rating was very high 5 and could be due to salinity, CO2, fluid flow rate
... Show MoreIn this work, studying the effect of ethylenediamine as a corrosion inhibitor was investigated for carbon steel in aerated HCl solution in range of 0.1-1N under dynamic conditions, i.e., rotational velocity of 400–1200 rpm in the temperature range 35 – 65 ºC. Weight loss method was employed in absence and presence of the inhibitor as an adsorption type in concentration range 1000 – 5000 ppm using rotating cylinder specimens. The experimental results showed that corrosion rate in absence and presence of inhibitor is increased with increasing temperature, rotational velocity and concentration of acid. It is decreased with increasing inhibitor concentration for the whole range of temperature, rotational velocity and concentrati
... Show MoreThe corrosion behavior of carbon steel at different temperatures 100,120,140 and 160 Cͦ under different pressures 7,10 and 13 bar in pure distilled water and after adding three types of oxygen scavengers Hydroquinone, Ascorbic acid and Monoethanolamine in different concentrations 40,60 and 80 ppm has been investigated using weight loss method. The carbon steel specimens were immersed in water containing 8.2 ppm dissolved oxygen (DO) by using autoclave. It was found that corrosion behavior of carbon steel was greatly influenced by temperature with high pressure. The corrosion rate decreases, when adding any one of oxygen scavengers. The best results were obtained at a concentration of 80 ppm of each scavenger. It was observed that
... Show MoreRotating cylinder electrode (RCE) is used . in weight loss technique , the salinity is 200000 p.p.m, temperatures are (30,5060,7080Co) . the velocity of (RCE) are (500,1500,3000 r.p.m). the water cut (30% , 50%). The corrosion rate of carbon steel increase with increasing rotating cylinder velocity. In single phase flow, an increase im rotational velocity from 500 to 1500 r.p.m, the corrosion rate increase from 6.88258 mm/y to 10.11563 mm/y respectively.
In multiphase flow, an increase in (RCE) from 500 to 1500 r.p.m leads to increase in corrosion rate from 0.786153 to 0.910327 mm/y respectively. Increasing brine concentration leads to increase in corrosion rate at water cut 30%.
The aim of the work is synthesis and characterization of bidentate ligand [3-(3-acetylphenylamino)-5,5-dimethylcyclohex-3-enone][HL], from the reaction of dimedone with 3-amino acetophenone to produce the ligand [HL], the reaction was carried out in dry benzene as a solvent under reflux. The prepared ligand [HL] was characterized by FT-IR, UV-Vis spectroscopy, 1H, 13C-NMR spectra, Mass spectra, (C.H.N) and melting point. The mixed ligand complexes were prepared from ligand [HL] was used as a primary ligand while 8-hydroxy quinoline [HQ] was used as a secondary ligand with metal ion M(Π).Where M(Π) = (Mn ,Co ,Ni ,Cu ,Zn ,Cd and Pd) at reflux ,using ethanol as a solvent, KOH as a base. Complexes of the composition [M(L)(Q)] with (1
... Show MoreThe azo ligand obtained from the diazotization reaction of 2-aminobenzothiazole and 4- nitroaniline yielded a novel series of complexes with Co(II), Ni(II), Cu(II), and Zn(II) ions. The complexes were investigated using spectral techniques such as UV-Vis, FT-IR, 1H and 13C NMR spectroscopic analyses, LC-MS and atomic absorption spectrometry, electrical conductivity, and magnetic susceptibility. The molar ratio of the synthesized compounds was determined using the ligand exchange ratio, which revealed the metal-ligand ratios in the isolated complexes were 1:2. The synthesized complexes were tested for antimicrobial activity against S. aureus, E. coli, C. albicans, and C. tropicalis bacterial species. Additionally, their binding affinities we