This work describes, selenium (Se) films were deposited on clean glass substrates by dc planar magnetron sputtering technique.The dependence of sputtering deposition rate of Se film deposited on pressure and DC power has been studied. The optimum argon pressure has range (4x10-1 -8x10-2 )mbar. The optical properties such as absorption coefficient (α) was determined using the absorbance and transmission measurement from UnicoUV-2102 PC spectrophotometer, at normal incidence of light in the wavelength range of 200-850 nm. And also we calculated optical constants(refractive index (n), dielectric constant (εi,r), and Extinction coefficient (κ) for selenium films.
Piroxicam is a non-steroidal anti-inflammatory drug (NSAID) used in the treatment of musculo-skeletal and joint disorders. The problem with this drug is its poor solubility in water and hence poor bioavailability after oral administration. In order to improve its solubility and dissolution behavior, hydrophilic additives such as starch, lactose, superdisintegrants including crospovidone (C.P), cross carmellose sodium (CCS), and sodium starch glycolate (SSG) were physically dry mixed with the drug by simple trituration. The improvement in the solubility in 0.1 N HCl was obtained as the amount of starch or lactose increased in the physical mixture, while for superdisintegrants, they further improve the solubility when they are present in s
... Show MorePAN/PMMA) with different blend ratios (80/20, 75/25,70/30,65/35, and 60/40) wt% undoped and doped with various lithium (Li) salts (LiCO3, Li2SO4H2O, and LiCl) at 20 wt %. Different techniques were employed to investigate the composition and optical properties of the prepared blend samples undoped and doped with Lithium salts like FT-IR and UV-Visible spectroscopies. The optical properties analysis declared that the energy gap increased from (4.0 eV to 4.20 eV) by increasing of PMMA ratio from 20 to 40 wt %. In contrast, the energy gap reduced and shifted toward the low energy side by adding lithium salts; the minimum energy gap value was 2 eV obtained from 65 % PAN and 35 % PMMA doped with Li2CO3. The optical constants were determ
... Show MoreThin films of GexS1-x were fabricated by thermal evaporating under vacuum of 10-5Toor on glass substrate. The effect of increasing of germanium content (x) in sulfide films on the electrical properties like d.c conductivity (σDC), concentration of charge carriers (nH) and the activation energy (Ea) and Hall effect were investigated. The measurements show that (Ea) increases with the increasing of germanium content from 0.1to0.2 while it get to reduces with further addition, while charge carrier density (nH) is found to decrease and increase respectively with germanium content. The results were explained in terms of creating and eliminating of states in the band gap
Thin films of ZnSxSe1-x with different sulfide content(x)
(0, 0.02, 0.04, 0.06, 0.8, and 0.1), thickness (t) (0.3, 0.5, and 0.7 μm) and annealing temperature (Ta) (R.T 373 and 423K) were fabricated by thermal evaporating under vacuum of 10-5 Toor on glass substrate. The results show that the increasing of sulfide content (x)and annealing temperature lead to decrease the d.c conductivity σDC of and concentration of charge carriers (nH) but increases the activation energy (Ea1,Ea2), while the increasing of t increases σDC and nH but decrease (Ea1,Ea2). The results were explained in different terms
Rare earth elements (Cerium, Lanthanum and Neodymium) doped CdS thin films are prepared using the chemical Spray Pyrolysis Method with temperature 200 oC. The X-ray diffraction (XRD) analysis refers that pure CdS and CdS:Ce, CdS:La and CdS:Nd thin films showed the hexagonal crystalline phase. The crystallite size determined by the Debye-Scherrer equation and the range was (35.8– 23.76 nm), and it was confirmed by field emission scanning electron microscopy (FE-SEM). The pure and doped CdS shows a direct band gap (2.57 to 2.72 eV), which was obtained by transmittance. The room-temperature photoluminescence of pure and doped CdS shows large peak at 431 nm, and two small peaks at (530 and 610 nm). The Current – voltage measurement in da
... Show MoreOwing to their cost-effectiveness and the natural abundance of magnesium, magnesium-ion batteries (MIBs) were introduced as encouraging alternatives to Lithium-ion batteries. Following the successful synthesis of carbon nano-tube, its B and N doped derivatives which were doped with B and N enjoyed the attention of researchers as novel anode materials (AM) for MIBs. Here, we investigated a BC2N nano-tube (BC2NNT) as an encouraging AM for MIBs. To have a deeper understanding of the electrochemical properties, cycling stability, specific capacity (SC) and the adsorption behavior of this nano-tube, first-principles density functional theory computations were performed. By performing NMR calculations, we identified two types of non-aromatic hexa
... Show MoreThe optical detectors which had been used in medical applications, and especially in radioactive treatments, need to be modified studied for the effects of radiations on them. This study included preparation of the MnS thin films in a way that vacuum thermal evaporation process at room temperature 27°C with thickness (400+-10nm) nm and a sedimentation rate of 0.39nm/sec on glass floors. The thin films prepared as a detector and had to be treated with neutron irradiation to examine the results gained from this process. The results decay X-ray (XRD) showed that all the prepared thin films have a multi-crystalline structure with the dominance of the direction (111), the two samples were irradiated with a neutron irradiation source (241Am-9Be)
... Show MoreIn this study, thin flms containing titanium dioxide (TiO₂), iron (III) oxide (Fe2O3) and cerium oxide (CeO2), with varying Fe2O3:CeO2 concentrations ranging from 0 to 30 wt% and 10 wt% gold nanoparticles (AuNPs), were prepared on glass using chemical spray pyrolysis. The structural, morphological, and sensing properties of the prepared thin flms were examined. XRD analysis revealed that a phase transformation occurred based on the dopant concentration: flms with x = 0 or 0.1 formed a polycrystalline anatase structure, whereas those with intermediate concentrations (x = 0.15 or 0.20) were amorphous. At higher doping concentrations (x = 0.25, 0.30), the structure developed a hematite Fe2O3, CeO2 and Au phase. Morphologicall
... Show More