Iron-Epoxy composite samples were prepared by added
different weight percentages (0, 5, 10, 15, and 20 wt %) from Iron
particles in the range of (30-40μm) as a particle size. The contents
were mixed carefully, and placed a circular dies with a diameter of
2.5 cm. Different mechanical tests (Shore D Hardness, Tensile
strength, and Impact strength ) were carried out for all samples. The
samples were immersed in water for ten weeks, and after two weeks
the samples were take-out and drying to conducting all mechanical
tests were repeated for all samples. The hardness values increased
when the Iron particle concentration increased while the Impact
strength is not affected by the increasing of Iron particles
concentration. The tensile strength results reveal that the tensile
strength and the strain values of composite samples decreases when
the Iron particles concentration increase. After conducted
immersion processes the results of hardness are reduced wears the
results of tensile strength and the impact strength are increased.
In this research we study the effect of UV radiation on pure PC samples and doped samples with plasticizer (DOP) for different exposure times (6, 12, 18, 24h). The study have been made on the change in the IR spectra causes by the UV radiation on both kinds of samples, besides the morphology changes were also studied by the optical microscope. From the results we conclude that the increasing of exposure causes the elaboration of CO2 and C2 gases.
Nanocrystalline micro-mesoporous ZSM/MCM-41 composite was synthesized using alkaline treatment method and two step of crystallization in poly tetraflouroethylene (PTFE) lined autoclave. The synthesized zeolites was characterized by X-Ray diffraction (XRD), Scanning electron microscopy (SEM), Transmission electron microscopy (TEM), Atomic force microscopy (AFM), Fourier transport infrared (FTIR), and N2 adsorption-desorption (BET). It was approved that the best results for alkaline leaching can be got with 1.5M NaOH solution. High surface (BET) area of 630 m2/g with pore volume of 0.55 cm3/g has been got. AFM reports showed a nano-level size for average particle size of 50nm.
It is suitable to use precast steel-concrete composite beams to quickly assemble a bridge or a building, particularly in isolated regions where cast-in-situ concrete is not a practical option. If steel-concrete composite beams are designed to allow demountability, they can also be extremely useful in the aftermath of natural disasters, such as earthquakes or flooding, to replace damaged infrastructure. Furthermore, rapid replacement of slabs is extremely beneficial in case of severe deterioration due to long-term stressors such as fatigue or corrosion. The only way to rapidly assemble and disassemble a steel-concrete composite structure is to use demountable shear connectors to connect/disconnect the steel beams to/from the concrete slab. I
... Show MoreIn Iraq, the risk of soil pollution by petroleum products increases with the growth of oil exploration, production and shipping large quantities of oil through pipelines over thousands of kilometers. Numerous oil spills have been documented recently in many sites due to damage in the oil industry infrastructures, which have led to soil contamination causing serious environmental hazards and deterioration to the soil and its engineering properties. So, it is essential to investigate the impact of oil leakage through the soil stratum consequently, assessing the eligibility of the contaminated soil for construction projects or identifying the appropriate treatment method. The paper investigates the general behaviour and the associated variatio
... Show MoreThe present study focused mainly on the buckling behavior of composite laminated plates subjected to mechanical loads. Mechanical loads are analyzed by experimental analysis, analytical analysis (for laminates without cutouts) and numerical analysis by finite element method (for laminates with and without cutouts) for different type of loads which could be uniform or non-uniform, uniaxial or biaxial. In addition to many design parameters of the laminates such as aspect ratio, thickness ratio, and lamination angle or the parameters of the cutout such as shape, size, position, direction, and radii rounding) which are changed to studytheir effects on the buckling characteristics with various boundary conditions. Levy method of classical lam
... Show MoreThe economical and highly performed anode material is the critical factor affecting the efficiency of electro-oxidation toward organics. The present study aimed to detect the best conditions to prepare Mn-Co oxide composite anode for the electro-oxidation of phenol. Deposition of Mn-Co oxide onto graphite substrate was investigated at 25, 30, and 35 mA/cm2 to detect the best conditions for deposition. The structure and the crystal size of the Mn-Co oxide composite electrode were examined by using an X-Ray diffractometer (XRD), the morphological properties of the prepared electrode were studied by scanning electron microscopy (SEM) and Atomic force microscopy (AFM) techniques, and the chemical composition of the various
... Show MoreSteps were taken to obtain the Kojic acid crystals from local fungal isolation A. flavus WJF81 by separating the fermentation products from the fungus mycelium from the production plant at the centrifuge at a speed of 5000 cycles for 10 minutes. The extraction was followed by ethyl acetate then supernatant concentrate by using rotary evaporator, and dried with heat oven 37ºC. Long, yellowish, pristine acid crystals were obtained that examined the optical microscope with a magnification force of 10x and 40x. The melting point of kojic acid was determined between 152.9-153.5 °C Results of the diagnosis of Kojic acid by applying High pressure liquid chromatography HPLC technique showed that the acid was at one peak, which was close to the
... Show MoreGypsum Plaster is an important building materials, and because of the availabilty of its raw materials. In this research the effect of various additives on the properties of plaster was studied , like Polyvinyl Acetate, Furfural, Fumed Silica at different rate of addition and two types of fibers, Carbon Fiber and Polypropylene Fiber to the plaster at a different volumetric rate. It was found that after analysis of the results the use of Furfural as an additive to plaster by 2.5% is the optimum ratio of addition to that it improved the flexural Strength by 3.18%.
When using Polyvinyl Acetate it was found that the ratio of the additive 2% is the optimum ratio of addition to the plaster, because it improved the value of the flexural stre