PVA, Starch/PVA, and Starch/PVA/sugar samples of different
concentrations (10, 20, 30 and 40 % wt/wt) were prepared by casting
method. DSC analysis was carried; the results showed only one glass
transition temperature (Tg) for the samples involved, which suggest
that starch/PVA and starch/PVA/sugar blends are miscible. The
miscibility is attributed to the hydrogen bonds between PVA and
starch. This is in a good agreement with (FTIR) results. Tg and Tm
decrease with starch and sugar content compared with that for
(PVA). Systematic decrease in ultimate strength, due to starch and
sugar ratio increase, is attributed to (PVA), which has more hydroxyl
groups that made its ultimate strength higher than that for
starch/PVA, and starch/PVA/sugar blends. It is observed from water
uptake tests that the solubility time decreases with starch ratio; it is
attributed to decrease in hydroxyl groups caused by PVA ratio
decrease. The inter- and inter-molecular bonds of the hydroxyl
groups enhanced the solubility process of the starch/PVA blends in
water. The water immersion causes hydrogen bonds (inter and
intermolecular bonds) to decompose, that increases the film
solubility. Water absorption and capacity of degradability are most
important in biodegradable materials. The results suggest the samples
that have undergone investigation, can be used for shopping, and
food packaging.
The study of soil burial for the sample at (3cm) depth, and at (13cm)
depth has exhibited weight loss increase with soil burial time. The
biodegradability rapidly increases at the first (6-7) weeks; it is found
that the weight loss at (3cm) depth is greater than that at (13cm) that
was attributed to the differences in the availability of oxygen ratio. It
is found that PVA undergoes lowest weight loss, the weight loss
changes with starch, and sugar content. In dry soil, the weight loss is
lower. The results proved that the biodegradation decreases with soil
burial time after seven weeks of burial. It is concluded that the
samples involved are biodegradable material that can be used for
packaging applications and biologically friendly synthetic polymer
blends to solve the solid waste accumulation problem.
Free cement refractory concrete is a type of refractory concrete with replacing alumina cement by bonding materials such as white kaolin, red kaolin and fumed silica. The free cement refractory concrete used in many applications like Petrochemicals, iron furnaces and cement production industries. The research clarifies the effect of steel fibers with two types crimped steel fibers and hooked steel
fibers with percentages 0.5%, 1% and 1.5% by volume from weight of bauxite aggregates. The additions of steel fibers with two types gave good properties in high temperatures where the specimens keep the dimension without failure and the properties made the best. the percentage of increasing for thermal conductivity was 44% for 1.5% crimped
The present investigation considers the effect of curing temperatures (30, 40, and 50˚C) and curing compound method on compressive strength development of high performance concrete, and compares the results with concrete cured at standard conditions and curing temperature (21˚C). The experimental results showed that at early ages, the rate of strength development at high curing temperature is greater than at lower curing temperature, the maximum increasing percentage in compressive strength is 10.83% at 50C˚ compared with 21C˚ in 7days curing age. However, at later ages, the strength achieved at higher curing temperature has been less, and the maximum percentage of reduction has been 5.70% at curing temperature 50C˚ compared with 21
... Show MoreDespite widespread agreement on the beneficial nature of hydrated lime (HL) addition to asphalt concrete mixes, understanding of the effect of HL particle size is still limited. Previous investigations have focused mainly on two different size comparisons, and so certain guidance for a practical application cannot yet be produced. This study investigates three distinct sizes of HL, in the range of regular, nano, and sub-nano scales, for their effects on the properties of modified asphalt concretes. Five different percentages of HL as a partial replacement of ordinary limestone filler in asphalt concrete mixes were studied for wearing course application purposes. Experimental tests were conducted to evaluate the mechanical properties
... Show MoreA recently reported Nile red (NR) dye conjugated with benzothiadiazole species paves the way for the development of novel organic-based sensitizers used in solar cells whose structures are susceptible to modifications. Thus, six novel NR structures were derived from two previously developed structures in laboratories. In this study, density functional theory (DFT) calculations and time-dependent DFT (TD-DFT) were used to determine the optoelectronic properties of the NR-derived moieties such as absorption spectra. Various linkers were investigated in an attempt to understand the impact of π-linkers on the optoelectronic properties. According to the findings, the presence of furan species led to the planarity of the molecule and a reduction
... Show MoreIn this research, a novel synthesis of CaONPs has been developed via an environmentally friendly, green method. Garlic extract (Allium sativum) was used as a green-reducing and stabilizing agent for CaONPs. The average particle size of CaONPs was approximately 24.42 nm. The synthesized CaONPs were identified by using Fourier transform infrared (FT-IR) spectroscopy, U.V.-vis spectrum, X-ray diffraction (XRD), Field Emission-Scanning Electron Microscopy (FE-SEM), Transmission Electron Microscopy, transmission electron microscopy (TEM), Energy Dispersive X-ray spectroscopy (EDX), Atomic Force Microscopy (AFM), and zeta potential (Zp) analysis. The current study highlights the notable applications for CaONPs. First, an antimicrobial assay revea
... Show MoreIn this paper, two elements of the multi-input multi-output (MIMO) antenna had been used to study the five (3.1-3.55GHz and 3.7-4.2GHz), (3.4-4.7 GHz), (3.4-3.8GHz) and (3.6-4.2GHz) 5G bands of smartphone applications that is to be introduced to the respective US, Korea, (Europe and China) and Japan markets. With a proposed dimension of 26 × 46 × 0.8 mm3, the medium-structured and small-sized MIMO antenna was not only found to have demonstrated a high degree of isolation and efficiency, it had also exhibited a lower level of envelope correlation coefficient and return loss, which are well-suited for the 5G bands application. From the fabrication of an inexpensive FR4 substrate with a 0.8 mm thickness level, a loss tang
... Show More