PVA, Starch/PVA, and Starch/PVA/sugar samples of different
concentrations (10, 20, 30 and 40 % wt/wt) were prepared by casting
method. DSC analysis was carried; the results showed only one glass
transition temperature (Tg) for the samples involved, which suggest
that starch/PVA and starch/PVA/sugar blends are miscible. The
miscibility is attributed to the hydrogen bonds between PVA and
starch. This is in a good agreement with (FTIR) results. Tg and Tm
decrease with starch and sugar content compared with that for
(PVA). Systematic decrease in ultimate strength, due to starch and
sugar ratio increase, is attributed to (PVA), which has more hydroxyl
groups that made its ultimate strength higher than that for
starch/PVA, and starch/PVA/sugar blends. It is observed from water
uptake tests that the solubility time decreases with starch ratio; it is
attributed to decrease in hydroxyl groups caused by PVA ratio
decrease. The inter- and inter-molecular bonds of the hydroxyl
groups enhanced the solubility process of the starch/PVA blends in
water. The water immersion causes hydrogen bonds (inter and
intermolecular bonds) to decompose, that increases the film
solubility. Water absorption and capacity of degradability are most
important in biodegradable materials. The results suggest the samples
that have undergone investigation, can be used for shopping, and
food packaging.
The study of soil burial for the sample at (3cm) depth, and at (13cm)
depth has exhibited weight loss increase with soil burial time. The
biodegradability rapidly increases at the first (6-7) weeks; it is found
that the weight loss at (3cm) depth is greater than that at (13cm) that
was attributed to the differences in the availability of oxygen ratio. It
is found that PVA undergoes lowest weight loss, the weight loss
changes with starch, and sugar content. In dry soil, the weight loss is
lower. The results proved that the biodegradation decreases with soil
burial time after seven weeks of burial. It is concluded that the
samples involved are biodegradable material that can be used for
packaging applications and biologically friendly synthetic polymer
blends to solve the solid waste accumulation problem.
Focusing on the negative role of default risk on banks, as it is one of the most important risks facing banks, which are difficult to determine accurately, and its reflection on the indicators of profitability of cash flows. The increasing competition between banks led to an increase in the credit facilities granted by banks, and was accompanied by an increase in exposure to the risks of default, which led to an impact on the level of performance of banks in terms of achieving the required return according to the levels of high competition. Therefore, the problem of this study focused on the extent to which the risk indicators of default affect the profitability indicators of the cash flows of the banks research sample in the profit
... Show MorePurpose: This study aimed to compare the stability and marginal bone loss of implants inserted with flapped and flapless approaches 8 weeks after surgery and 3 months after loading. Material and Methods: Thirty SLActive implants were inserted in 11 patients and early loaded with final restoration 8 weeks after healing period. The stability values determined by Osstell and the marginal bone loss measured by CBCT at the initial time (1st) and 8 weeks of the healing period (2nd) and 3 months after loading (3rd). Results: The overall survival rate was 100%. A significant increase in the 3rd implant stability value in the age of ˂ 40. A significant decrease in the 2nd implant stability value in both gender and traumatic zone with a flapless app
... Show MoreThe aim of the research is to identify an appropriate training method that raises the levels of immune globulins (IgA, IgM, IgG) and white blood cells and the effect of training by (HIT) method using resistance (weights) as a training curriculum that increases immunity and ensures the continuation of the pills after the return of activity from the stone The response to the Covid-19 epidemic among amateur weightlifters, the researchers relied on the method of trace analysis in an experimental way by conducting a pre-, medial and post-test with the same experimental one agroup on a sample of amateur weightlifters in the Fury private hall for weightlifting and body building in Adhamiya, the number of sample members reached (15 players) who int
... Show MoreCdO:NiO/Si solar cell film was fabricated via deposition of CdO:NiO in different concentrations 1%, 3%, and 5% for NiO thin films in R.T and 723K, on n-type silicon substrate with approximately 200 nm thickness using pulse laser deposition. CdO:NiO/n-Si solar cell photovoltaic properties were examined under 60 mW/cm2 intensity illumination. The highest efficiency of the solar cell is 2.4% when the NiO concentration is 0.05 at 723K.
Knowledge of the distribution of the rock mechanical properties along the depth of the wells is an important task for many applications related to reservoir geomechanics. Such these applications are wellbore stability analysis, hydraulic fracturing, reservoir compaction and subsidence, sand production, and fault reactivation. A major challenge with determining the rock mechanical properties is that they are not directly measured at the wellbore. They can be only sampled at well location using rock testing. Furthermore, the core analysis provides discrete data measurements for specific depth as well as it is often available only for a few wells in a field of interest. This study presents a methodology to generate synthetic-geomechani
... Show MoreAn aromatic ester containing two azo groups namely p-nitro phenyl azo-β-naphthyl-(4'-azobenzoic acid)-4-benzoate was synthesized by esterfiaction of 4,4'-azo dibenzoic acid with p-nitro phenyl azo-β-naphthol. Synthesized ester was characterized by CHN-Elemental analysis, FTIR, 1H NMR and 13C NMR. A modified PVA polymer was obtained by grafting 10 g of PVA-polymer via partial esterification with (2, 3, 4 g) p-nitro phenyl azo-1-naphthyl-4-azobenzoic acid)-4-azo benzoate. Grafting PVA-polymer behaviours was studied, by physical measurements (solubility, swelling), thermal properties (DSC) and tensile.
The study was aimed to determine the coordinates of the points were measured by different ways and different instruments, the most precise way using the differential global positioning system (DGPS) that will be the reference measurements in comparison, less precise way using navigator GPS. Google earth (pro.), and the other applications of GPS mobile ( Samsung and I-phone). In this research (8 points) were chosen that are occasional in location. The comparison of the different observations can give us an idea of the extent to which the accuracy of the observations differs from the different devices used in the observing, as well as through the knowledge of the best device and the best way to measure coordinates accurately t
... Show More