Thin films of pure WO3 and the binary systems of TiO2:WO3,MoO3:WO3,Cr2O3:WO3, and SnO2:WO3 were prepared by pulsed laser deposition method. The single and binary compounds were sintered at 1273K for five hours. The deposition were done under vacuum of 2x10-2 Torr at various substrates like glass and single crystal silicon wafer with negative conductance at ambient temperature thickness of ≍150 nm. The structures and morphology of pure WO3 and the binary systems TiO2:WO3,MoO3:WO3,Cr2O3:WO3, and SnO2:WO3 compounds and the deposited thin films were studied by X–ray diffraction and AFM atomic force microscope. The optical properties imply optical energy gap as well as optical constants for all the single and binary system were determined and discussed. The results of gas sensing measurements to NO2 gas showed that MoO3:WO3 sensors prepared on n- Si substrate showed maximum sensitivity (194.5%) at operating temperature 300K.
A total of (90) blood samples were collected from male patients infected with Toxoplasmosis who recovered from COVID- 19 and attended Kamal Alsamiraai Hospital from 15 January to 15 September 2021. We measured anti-Toxoplasma antibodies (IgG and IgM) detected by ELISA, whereas Anti-COVID-19 antibodies (IgG and IgM) were estimated using Elisa and Afilias. The semen characteristics were also studied among fertile, healthy individuals (control group) and sub-fertile patients. Results showed that the mean sperm count was high among the control group (40.5±1.3x 106/ml) compared with that of the sub-fertile patients (10.3±1.75 and 8.8±1.9 x 106/ml for oligozoospermia, and oligoasthenozoospermia respectively), and it was the highest (44.7±1.4
... Show MoreThe characterization of ZnO and ZnO:In thin films were confirmed by spray pyrolysis technique. The films were deposited onto glass substrate at a temperature of 450°C. Optical absorption measurements were also studied by UV-VIS technique in the wavelength range 300-900 nm which was used to calculate the optical constants. The changes in dispersion and Urbach parameters were investigated as a function of In content. The optical energy gap was decreased and the wide band tails were increased in width from 616 to 844 eV as the In content increased from 0wt.% to 3wt.%. The single–oscillator parameters were determined also the change in dispersion was investigated before and after doping.
Pure SnSe thin film and doped with S at different percentage (0,3,5,7)% were deposited from alloy by thermal evaporation technique on glass substrate at room temperature with 400±20nm thickness .The influences of S dopant ratio on characterization of SnSe thin film Nano crystalline was investigated by using Atomic force microscopy(AFM), X-ray diffraction (XRD), energy dispersive spectroscopy (EDS), Hall Effect measurement, UV-Vis absorption spectroscopy to study morphological, structural, electrical and optical properties respectively .The XRD showed that all the films have polycrystalline in nature with orthorhombic structure, with preferred orientation along (111)plane .These films was manufactured of very fine crystalline size in the ra
... Show MoreIn this work, As60Cu40-xSex thin films were synthesized, and the pulsed laser deposition method was used to study the effected partial replacement of copper with selenium. The electrical characteristics and optical characteristics, as indicated by the absorbance and transmittance as a function of wavelength were calculated. Additionally, the energy gap was computed. The electrical conductivity of the DC in the various conduction zones was calculated by measuring the current and voltage as a function of temperature. Additionally, the mathematical equations are used to compute the energy constants, electron hopping distance, tail width, pre-exponential factor, and density of the energy states in variation zones (densities of the energ
... Show MoreNano crystalline copper sulphide (Cu2S) thin films pure and 3% Bi doped were deposited on glass substrate by thermal evaporation technique of thickness 400±20 nm under a vacuum of ~ 2 × 10− 5 mbar to study the influence of annealing temperatures ( as-deposited, and 573) K on structural, surface morphology and optical properties of (Cu2S and Cu2S:3%Bi). (XRD) X-ray diffraction analysis showed (Cu2S and Cu2S:3%Bi) films before and after annealing are polycrystalline and hexagonal structure. AFM measurement approves that (Cu2S and Cu2S:3%Bi) films were Nano crystalline with grain size of (105.05-158.12) nm. The optical properties exhibits good optical absorption for Cu2S:3%Bi films. Decreased of optical band gap from 2.25 to 2 eV after dop
... Show MoreIn this work, InSe thin films were deposited on glass substrates by thermal evaporation technique with a deposit rate of (2.5∓0.2) nm/sec. The thickness of the films was around (300∓10) nm, and the thin films were annealed at (100, 200 and 300)°C. The structural, morphology, and optical properties of Indium selenide thin films were studied using X-ray diffraction, Scanning Electron Microscope and UV–Visible spectrometry respectively. X-ray diffraction analyses showed that the as deposited thin films have amorphous structures. At annealing temperature of 100°C and 200°C, the films show enhanced crystalline nature, but at 300°C the film shows a polycrystalline structure with Rhombohedral phas