In this study, thin film of pure zinc oxide (ZnO) and ZnO doped with Ga2O3 films with different concentrations (0, 0.03, 0.05, 0.07 and 0.09)wt% were prepared by pulsed laser deposition. The powder mixture was then sintered in a furnace at 1273 K for 5 h. The resulting powders were thoroughly ground and then pressed using a special press to form discs with a diameter of 1 cm and a thickness of 0.5 cm. The deposition was carried out under a vacuum of 2.5×10−2 mbar on various substrates, including glass for AFM measurements and n-type crystalline silicon wafers for the gas sensor. AFM results revealed a progressive increase in both grain size and roughness with moderate doping and irregularity at high doping levels. Gas-sensing measurements for the oxidizing gas (NO2) and the reducing gas (H2S) were conducted by measuring resistance in the absence and presence of each gas. The prepared sensors (ZnO: Ga2O3) on n-type silicon substrates showed maximum sensitivity (1076.31) at a doping ratio of 3% and an operating temperature of 373 K for nitrogen dioxide gas, with a response time 31.5 s, while the highest sensitivity to H2S gas was 24.53 for pure ZnO at operating temperature of 373 K with a response time of 33.3s. The sensor exhibited remarkable selectivity for NO2 gas due to its oxidizing nature; it extracts electrons from the conduction band of zinc oxide (ZnO), which leads to the expan- sion of the depletion layer and a significant change in electrical resistance.
In this work the design and construction of a flash photolysis pulsed HCl laser was presented. The parameters of the pumping source and discharge current density was obtained, which sufficient to shift the flash lamp spectrum towards uv portion of spectrum. The maximum pulse laser energy parameters was measured. Total pressure and ratio of active gases to optimized the output pulse energy were measured , where at 125 mbar of total pressure and 1:7:14 Cl2:H2: He ratio, the laser energy was measured to be 200 mJ at pumping four flash lamps energy in the order of 6400J .The resonator consists of copper a near hemispherical mirror with the radius of curvature 3m coated by gold and reflectivity 98%,the output coupler sapphire mirror of
... Show MoreIn this work, nanostructure zinc sulfide (ZnS) thin films at temperature of substrate 450 oC and thickness (120) nm have been produced by chemical spray pyrolysis method. The X-Ray Diffraction (XRD) measurements of the film showed that they have a polycrystalline structure and possessed a hexagonal phase with strong crystalline orientation of (103). The grain size was measured using scanning electron microscope (SEM) which was approximately equal to 80 nm. The linear optical measurements showed that ZnS nanostructure has direct energy gap. Nonlinear optical properties experiments were performed using Q-switched 532 nm Nd:YAG laser Z-scan system. The nonlinear refractive index (n2) and nonlinear absorption coefficient (β) estimated for Z
... Show MoreThin films ZrO2: MgO nanostructure have been synthesized by a radio frequency magnetron plasma sputtering technique at different ratios of MgO (0,6, 8 and 10)% percentage to be used as the gas sensor for nitrogen dioxide NO2. The samples were investigated by X-ray diffraction (XRD), atomic force microscopy (AFM), scanning electron microscopy (SEM), energy-dispersive X-ray (EDX) and sensing properties were also investigated. The average particle size of all prepared samples was found lower than 33.22nm and the structure was a monoclinic phase. The distribution of grain size was found lower than36.3 nm and uninformed particles on the surface. Finally, the data of sensing properties have been discussed, where the
... Show MorePure cadmium oxide films (CdO) and doped with zinc were prepared at different atomic ratios using a pulsed laser deposition technique using an ND-YAG laser from the targets of the pressed powder capsules. X-ray diffraction measurements showed a cubic-shaped of CdO structure. Another phase appeared, especially in high percentages of zinc, corresponding to the hexagonal structure of zinc. The degree of crystallinity, as well as the crystal size, increased with the increase of the zinc ratio for the used targets. The atomic force microscopy measurements showed that increasing the dopant percentage leads to an increase in the size of the nanoparticles, the particle size distribution was irregular and wide, in addition, to increase the surfac
... Show MoreIn this work, PAni nanofibers (NFs) are successfully synthesized via hydrothermal method. The structural, surface morphological, optical, electrical and H2S gas sensing properties have been investigated for PAni thin films deposited by spin coating technique. The XRD pattern reveals crystalline nature of PAni NFs with crystallite size of 9.2 nm. The SEM image of Polyaniline clearly indicates that the polymer possesses nanofiber like structure. The optical properties show that the optical energy gap follows allowed direct electronic transition calculated using Tauc’s equation. Intense hotoluminescence (PL) peaks at 309, 340 and 605 nm are observed. The electrical properties such as D.C. conductivity and Hall effect have been studied wher
... Show MoreIn this work, lead oxide nanoparticles were prepared by laser ablation of lead target immersed in deionized water by using pulsed Nd:YAG laser with laser energy 400 mJ/pulse and different laser pulses. The chemical bonding of lead oxide nps was investigated by Fourier Transform Infrared (FTIR); surface morphology and optical properties were investigated by Scanning Electron Microscope (SEM) and UV-Visible spectroscopy respectively, and the size effect of lead oxide nanoparticles was studied on its antibacterial action against two types of bacteria Gram-negitive (Escherichia coli) and Gram-positive (Staphylococcusaurus) by diffusion method. The antibacterial property results show that the antibacterial activity of the Lead oxide NPs was
... Show More